High Molecular Weight (HMW) Rubber is a rather challenging material to analyze. They may come in the form of EPR, EPDM, PIB, SBS, Polyisoprene or Natural Rubber etc. This class of material is important to the industrial sector because of its high strength and resilience. The saturated versions also excel in heat, chemical and environment resistance. The purpose of this application note is to show that we can obtain repeatable data for a variety of HMW Rubber samples.
Solvent |
Xylenes |
Sample Concentration |
0.025 g/dL |
Prep Temperature |
80C |
Dissolution Time |
16 Hours |
Filtration |
3.1 um Glass Fiber |
Analysis Temperature |
80C |
Sample A IV (dL/g) |
Sample B IV (dL/g) |
Sample C IV (dL/g) |
|
Injection 1 |
2.8146 |
2.4966 |
2.6226 |
Injection 2 |
2.8156 |
2.4957 |
2.6261 |
Average |
2.8151 |
2.4962 |
2.6244 |
SD |
0.0005 |
0.0005 |
0.0018 |
RSD |
0.02% |
0.02% |
0.07% |
The excellent data clearly shows that the actual IV measurement is extremely simple. The most important aspect of this analysis is sample prep. All the conditions were carefully chosen to yield good polymer solutions and repeatable IV values.
In addition to the precision of the data demonstrated above, the relative viscometer presents an easy opportunity to automate a particularly laborious task. Automation can range from a simple autosampler system to fully automated Vortex operation.
In addition to the precision of the data demonstrated above, the relative viscometer presents an easy opportunity to automate a particularly laborious task. Automation can range from a simple autosampler system to fully automated Vortex operation.